TIG ALUMINUM .063" LAP JOINT 60HZ
scroll down for settings
WELD PROCESS = TIG, GTAW, GAS TUNGSTEN ARC WELDING
METAL TYPE = ALUMINUM 6061
THICKNESS = .063"
WELD TYPE = FILLET
JOINT TYPE = LAP JOINT
POSITION = 2F
AMPERAGE = 80 AMPS ON MACHINE CONTROLLED BY FOOT PEDAL
TUNGSTEN = 2% LANTHANATED, 3/32"
FILLER WIRE = 1/16” 4043
POLARITY = AC
GAS FLOW = 15 CFH argon
CUP SIZE = 5
ADDITIONAL SETTINGS = AC BALANCE 30% CLEANING, AC FREQ 60HZ
PRE FLOW = .5 SEC
POST FLOW = 7 SEC
TIPS: KEEP A FAIRLY TIGHT ARC AND WATCH TORCH ANGLE
Aim for an arc length that is equal or less than the diameter of your tungsten electrode.Torch angle can be forgiving provided your arc length is tight.
You might like these
A good Test for any Tig Welding Machine arc starts is welding Coke Cans
The best Aluminum Welding Training you can get on your own - How to Get better at Tig Welding
Videos on Tig Welding Aluminum and learning how to tig weld
Enjoy this page? Please pay it forward. Here's how...
Would you prefer to share this page with others by linking to it?
- Click on the HTML link code below.
- Copy and paste it, adding a note of your own, into your blog, a Web page, forums, a blog comment,
your Facebook account, or anywhere that someone would find this page valuable.