WELD PROCESS = GMAW, SHORT CIRCUIT MIG, GAS METAL ARC, BARE WIRE MIG
METAL TYPE = CARBON STEEL, COLD ROLLED STEEL, AISI 1010
THICKNESS = 3/8” with 30 degree bevel
WELD TYPE = cover pass for open butt Groove weld
JOINT TYPE =Butt
POSITION = 3g vertical uphill
VOLTS = 17.7 volts
WIRE SPEED = 200 IPM
WIRE SIZE = .035"
POLARITY = DCEP
GAS FLOW = 20-25 CFH C25 GAS
CTWD = 3/8”-1/2"
FILLER METAL = ER70S6
ADDITIONAL SETTINGS =
TIPS:A relatively short stickout aka contact to work distance CTWD of 3/8” to 1/2" makes a big difference.
The technique shown is simple z weave that keeps arc on the leading edge of the puddle